Grade equivalence is a starting point, not a release. A conversion chart will tell you that ASTM Grade 2, Chinese TA2 and Werkstoff 3.7035 are “the same” titanium; the chemistry limits are not the same, and the certificate, condition and product standard are separate decisions. The clearest example is Grade 23: ASTM B265 calls it UNS R56407, while the implant standard ASTM F136 calls the same ELI alloy R56401 — a chart that prints only R56401 has copied the medical number onto an industrial grade. Under the current Chinese standard GB/T 3620.1–2016 the grades that truly match ASTM Gr1–Gr4 are TA1G–TA4G, not the restored TA1–TA4 labels most charts use. Boundary: this guide compares published nominal chemistry and standard scope, not design allowables; where reputable sources conflict, we name the conflict instead of choosing a side. The At a Glance table maps each claim to the field that must be written on a purchase order.
How to read the numbers in this article. We are a stockholder and light fabricator in Baoji, not a standards body. Every chemistry value below is attributed to the standard or producer source it came from. Values that sources disagree on — the aluminium ceiling for TC4, the Werkstoff number for ELI, minimum tensile by product form — are marked verify the revision rather than quietly selected. Where a source is a commercial cross-reference table rather than a published standard, we say so. That distinction is the entire point of this article.
| Claim on a chart | Typical wording | What actually differs | Cost if accepted at face value |
|---|---|---|---|
| Grade name | Gr2 / TA2 / 3.7035 | Nominal chemistry match only | A wrong material accepted on a PO |
| CP pure grades | Gr1–Gr4 differ by O and Fe | O 0.18 → 0.40 wt%; Fe 0.20 → 0.50 | A strength-driven grade substitution |
| Ti-6Al-4V | Gr5 / TC4 / 3.7165 | TC4 Fe ≤0.30% vs Gr5 Fe ≤0.40% | Less pitting margin in chlorides |
| ELI | Gr23 / TC4 ELI | R56407 (ASTM B series) or R56401 (F136); O 0.13, Fe 0.25 | Implant or cryogenic part rejected |
| Pd and Mo-Ni | Gr7=TA9=3.7235; Gr12=TA10=3.7105 | Pd 0.12–0.25; Ni 0.6–0.9, Mo 0.2–0.4 | Paying a Pd price for a CP grade |
| Product standard | B338 ≠ GB/T 3624; B861 ≠ GB/T 3625 | Heat-exchanger tube is GB/T 3625; seamless pipe is 3624 | Wrong test scope on the certificate |
| Aerospace | AMS 4928 vs B348 Gr5 | Fe 0.30 vs 0.40, H 0.0125 vs 0.015, mandatory UT | Airworthiness nonconformance |
| Certificate | EN 10204 3.1 vs 3.2 | 3.2 needs a named witness before manufacture | Lot rejected on receipt |
| Scope errors | EN 10088 = stainless; EN 485 = aluminium | Neither standard covers titanium | Specification rejected at review |
How to use this table: each row is a sentence you should never leave vague on a purchase order. A supplier who can state the chemistry edition, UNS number and certificate type without checking is worth a sample order.
A cross-reference table answers one narrow question: which name in another system describes roughly the same alloy? It does not answer whether that material can be released against your drawing, your certificate requirement or your corrosion allowance. That takes four more fields — chemistry edition, product standard, condition and inspection document — and those fields are where the money is.
Consider GB/T 3621 against ASTM B265. The two standards cover the same product form and broadly the same grades, but the chemistry edition and the acceptance tests are not interchangeable sentence for sentence. The same logic runs through every equivalence claim below. If you want the product background before the specification detail, start with our Titanium Plate overview; this article assumes you know the form and focuses on the designation.
Here is the working map, with the caveats marked. The UNS numbers are taken from the official scope of ASTM B265-20; the Werkstoff numbers are the ones most European stockists use. An asterisk means the mapping is disputed or version-dependent, and the dagger marks the implant number.
| ASTM grade | UNS | GB/T (correct) | Werkstoff | Nominal chemistry (wt%) |
|---|---|---|---|---|
| Gr1 | R50250 | TA1G | 3.7025 | CP Ti, O ≤0.18, Fe ≤0.20 |
| Gr2 | R50400 | TA2G | 3.7035 | CP Ti, O ≤0.25, Fe ≤0.30 |
| Gr3 | R50550 | TA3G | 3.7055 | CP Ti, O ≤0.35, Fe ≤0.30 |
| Gr4 | R50700 | TA4G | 3.7065 | CP Ti, O ≤0.40, Fe ≤0.50 |
| Gr5 | R56400 | TC4 | 3.7165* | Ti-6Al-4V, Al 5.5–6.75, V 3.5–4.5 |
| Gr7 | R52400 | TA9 | 3.7235 | Ti + Pd 0.12–0.25 |
| Gr9 | R56320 | TA18 | 3.7195 | Ti-3Al-2.5V |
| Gr12 | R53400 | TA10 | 3.7105 | Ti-0.3Mo-0.8Ni |
| Gr23 | R56407* / R56401† | TC4 ELI | 3.7165 / 3.7164* | Ti-6Al-4V ELI, O ≤0.13 |
Read the table as a shortlist, not a specification. The Werkstoff column is where most charts go wrong: Hempel and HSM use 3.7164 for aerospace AMS Grade 5 and 3.7165 for industrial ASTM Grade 5 and medical ELI, while many commercial charts reverse the pair. Both cannot be right, and ELI has no single unambiguous Werkstoff number. State the ASTM grade and revision instead of relying on the European number alone.
What people say: TA1 is Grade 1, TA2 is Grade 2, TA3 is Grade 3, TA4 is Grade 4. The table appears on hundreds of supplier sites, including our own industry’s trade pages.
What the standard actually says: Bao Ti Group’s analysis of GB/T 3620.1–2016, published by the standard-drafting team in Iron & Steel Vanadium Titanium (2022), sets out the history. The 2007 revision adopted grades TA1–TA4 from ISO 5832-2 and ASTM with matching chemistry. The 2016 revision restored the 1994 TA0–TA3 designations and renamed the 2007 set TA1G–TA4G, the G marking commercially pure titanium. So in the current standard the grades that truly correspond to ASTM Gr1–Gr4 are the G-suffixed ones. Under the restored labels, TA1 has an oxygen ceiling near 0.20% and sits close to Grade 2; under the 2007 set TA1G is 0.18% and matches Grade 1.
Why this is expensive: a mill certificate that says simply “TA2” does not tell you which chemistry edition applied at melt. The Bao Ti paper names the consequence directly — material standards issued after 2007 that were never revised still carry the old TA1 / TA2 / TA3 labels, so chemistry and mechanical properties can be mismatched. Their prevention is the line to copy into your PO: give the complete material standard number and confirm the chemistry edition, then write both into the contract. Our Grade 2 plate to ASTM B265 page states the ASTM side explicitly so the two can be reconciled.
The fastest way to remove this ambiguity is to send a complete designation on the first enquiry. These nine lines are what we ask for; copy them into your RFQ and any supplier can quote against the same basis.
|
What to send us for an exact titanium quote Copy these nine lines into your enquiry. A complete spec means a firm price on the first reply, not a second email asking for the grade. |
||||||||||||||||||||
|
||||||||||||||||||||
|
Ready? Copy the nine lines above into the Requirement Details box on our Request a Quotation page and we will come back with a firm price and a dispatch date within 24 hours. |
What people say: Grade 23 is UNS R56401. This is printed on most commercial equivalence charts, including well-known European stockists.
What ASTM says: the official scope of ASTM B265-20 lists Grade 23 as UNS R56407, describing it as Ti-6Al-4V with extra low interstitial elements. ASTM B348, B381 and B863 follow the B-series convention. R56401 belongs to ASTM F136, the specification for Ti-6Al-4V ELI alloy for surgical implant applications. The rule is simple: the product standard comes first, and the UNS follows it. A chart that lists only R56401 has taken a medical designation and applied it to an industrial grade.
What to write in the PO: name the standard you are certifying against, then the UNS. “Grade 23 per ASTM B348, UNS R56407, annealed” and “Ti-6Al-4V ELI per ASTM F136, UNS R56401” are two different orders with different melt, cleanliness and testing obligations. If the application is a load-bearing implant, a generic Grade 5 bar certificate is the wrong document regardless of what the equivalence chart says.
European drawings often carry a Werkstoff number instead of an ASTM grade, which is where the second dispute starts. Hempel Special Metals and the German Werkstoff database HSM describe 3.7164 as the Ti-6Al-4V grade specified to AMS for aerospace, and 3.7165 as the industrial ASTM variant — adding that 3.7165 is also used in medical technology with the ELI suffix and Grade 23 designation. METALCOR lists Grade 5 as 3.7164/65 and Grade 23 ELI as 3.7165. A large group of commercial charts states the reverse: Grade 5 is 3.7165 and Grade 23 is 3.7164.
What to do with the conflict: do not pick a side in a purchase order. Ask the customer which ASTM or AMS specification the Werkstoff number was derived from, and quote against that. If the drawing says 3.7165 with no standard, the honest answer is a question, not a confident conversion. This is one of the few places where a supplier who says “please confirm” is more credible than one who says “no problem”.
The clearest demonstration is Grade 2, the most traded titanium grade. Five systems all claim to describe the same commercially pure metal; their interstitial and iron ceilings are not the same.
| System | O max | Fe max | N max | C max | H max |
|---|---|---|---|---|---|
| ASTM Gr2 (B265 / B348) | 0.25 | 0.30 | 0.03 | 0.08 | 0.015 |
| Werkstoff 3.7035 (DIN) | 0.20 | 0.25 | 0.06 | 0.08 | 0.013 |
| GB TA2 | 0.25 | 0.30 | 0.05 | 0.10 | 0.015 |
| GOST BT1-0 | 0.20 | 0.30 | 0.04 | 0.07 | 0.010 |
| JIS Class 2 | 0.20 | 0.25 | 0.05 | — | 0.015 |
ASTM Gr2 permits up to 0.25% oxygen and 0.30% iron. DIN / Werkstoff 3.7035 permits only 0.20% oxygen and 0.25% iron but raises nitrogen to 0.06%. ISO 5832-2 CP2 sets its own oxygen value again. Each system can honestly call the material “Grade 2”, and a part made at the top of one range may sit outside another. For the corrosion-sensitive work that titanium tube usually sees, the practical rule is to request measured chemistry rather than rely on the grade name. Our EN 10204 3.1 mill certificate page shows the fields in which those measurements appear.
Now the alloy grades. TC4, Grade 5 and Grade 23 are close enough to be grouped in a sales conversation and different enough to matter in a specification.
| Element | TC4 (GB/T 3620.1) | Gr5 (ASTM B265 / B348) | Gr23 ELI (F136 / B series) |
|---|---|---|---|
| Al | 5.5–6.8* | 5.5–6.75 | 5.5–6.5 |
| V | 3.5–4.5 | 3.5–4.5 | 3.5–4.5 |
| Fe (max) | 0.30 | 0.40 | 0.25 |
| O (max) | 0.20 | 0.20 | 0.13 |
| N (max) | 0.05 | 0.05 | 0.03 |
| H (max) | 0.015 | 0.015 | 0.0125 |
| Tensile min (annealed) | per GB/T 3621 | 895 MPa* | 828 MPa (B series)* / 860 (F136)* |
The iron difference is the one to remember. ASTM Grade 5 allows up to 0.40% iron; TC4 is listed at 0.30%. The aluminium upper limit is published as 6.8 in some Chinese sources and 6.75 in ASTM, so verify the revision rather than writing either into a critical PO without checking. Grade 23 controls oxygen at 0.13%, iron at 0.25% and hydrogen at 0.0125% — and it is specified for toughness and cryogenic or implant service, not for extra strength.
The counter-intuitive fact: Grade 23's minimum tensile is lower than Grade 5's, roughly 828 MPa against 895 MPa for annealed product, with the figure varying by standard and form. Anyone describing ELI as “a stronger Grade 5” has misunderstood the reason the variant exists. If the design needs strength, cite Grade 5 with its condition; if it needs fracture toughness at low temperature or an implant-grade chemistry, cite ELI.
Even with the right grade, the product standard decides which tests are performed and which properties are guaranteed. Mapping one standard number to another by name is the third common error.
| Form | ASTM | GB/T | Note |
|---|---|---|---|
| Plate / sheet | B265 | GB/T 3621 | Direct equivalent in scope; chemistry still version-specific |
| Heat-exchanger tube | B338 | GB/T 3625 | Often wrongly mapped to 3624 |
| Seamless pipe | B861 | GB/T 3624 | General pipe, not condenser tube |
| Bar / billet | B348 | GB/T 2965 | Check condition: annealed vs cold-worked |
| Fittings | B363 | GB/T 27684 | The GB standard states no adopted ASTM equivalent |
| Forgings | B381 | GB/T 25137 / 16598 | Two GB standards split forgings and rings |
| Wire | B863 | GB/T 3623 | Filler wire adds AWS A5.16 requirements |
| Chemistry tolerance | — | GB/T 3620.2 | Use for arbitration on a disputed heat |
Two mappings are routinely inverted: heat-exchanger tube is GB/T 3625, while GB/T 3624 covers general seamless pipe; and the Titanium Fittings standard GB/T 27684–2011 states in its own record that it adopted no ASTM standard, borrowing only ASME B16.5 and B16.9 dimensions. A standard number that looks equivalent is therefore not proof of technical equivalence. When you order Titanium Fittings or AWS A5.16 filler wire, name the inspection requirements you expect in addition to the number.
These two specifications describe the same UNS R56400 alloy, which makes them a favourite for careless substitution. What changes is the envelope around it.
| Aspect | AMS 4928 | ASTM B348 Grade 5 |
|---|---|---|
| Melt practice | Multiple VAR required | No equivalent mandatory VAR schedule |
| Iron | Fe ≤0.30% | Fe ≤0.40% |
| Hydrogen | H ≤0.0125% | H ≤0.015% |
| Ultrasonic testing | AMS 2631 mandatory | Not a default requirement |
| Records | Beta transus and microstructure recorded | Not required by the base product standard |
| Section | Bars and forgings to 152 mm | Broader product-size coverage |
An ASTM B348 heat can pass its product standard and still fail AMS 4928 on iron, hydrogen or ultrasonic inspection. If the drawing names AMS 4928, the order must be quoted and certified to that revision. This is the fourth trap, and it is the one that most often turns a technically sound bar into an airworthiness nonconformance.
If a designation on your drawing is still ambiguous — a Werkstoff number without a standard, a grade without a revision — send it through our request a quotation page and a named engineer will return the ASTM grade, the chemistry edition and the certificate option within 24 hours.
The fifth trap sits at the medical boundary. ASTM F136 is the surgical-implant specification for Ti-6Al-4V ELI: it uses UNS R56401 and adds double or triple vacuum arc remelting, mandatory fatigue testing, ASTM F1440 microcleanliness and a yttrium limit of 0.005%. An industrial Grade 23 certificate to B348 or B265 does not contain those obligations. A well-documented case in the supply trade is a dental laboratory rejecting a lot described as “implant grade” because the supplier could not produce an ASTM F136 certificate of conformance.
China has its own implant standard, GB/T 13810, aligned with ISO 5832-2 and -3 for surgical implants. If you are importing a Chinese product for that market, the question is never “is it Grade 23?” but “which implant specification and which certificate of conformance?”. We will say plainly when an order belongs with a qualified implant chain rather than a general stockholder; that answer is more useful than a certificate that will be rejected at receiving inspection.
The sixth trap is a category error. EN 10204 defines types of inspection document: 2.1 a declaration of compliance, 2.2 a test report from the same production batch but not the delivered lot, 3.1 an inspection certificate signed by a manufacturer’s representative independent of production, and 3.2 the same inspection co-signed by a purchaser’s representative or a notified third party. The number indicates who signs, not how much was tested and certainly not which chemistry applies.
EN 10204 and ASTM are therefore complementary: a B348 mill test certificate is commonly issued as EN 10204 3.1. Two related scope errors are worth flagging because they appear on real enquiries: EN 10088 is the stainless-steel standard family, and EN 485 covers aluminium sheet and strip. Neither covers titanium. Citing either for a titanium grade is a scope error, not an alternative designation. A related name to avoid is “DIN 17025” — DIN EN ISO/IEC 17025 is laboratory accreditation, not a titanium grade standard.
There are orders where a conversion table should not be used at all. Naming them early is part of giving a straight answer.
| Condition | Why equivalence fails | What to do instead |
|---|---|---|
| Load-bearing implant or surgical device | Needs ASTM F67 / F136 + ISO 5832-2/-3 (GB/T 13810); industrial grade cannot be released against it | Source from a qualified implant chain with a certificate of conformance |
| Aerospace drawing naming an AMS number | The AMS envelope, not the grade name, controls melt, UT and records | Quote and certify to the named AMS revision |
| Cryogenic or fracture-critical service | ELI is specified for toughness; standard Gr5 is not a drop-in | Specify Gr23 / TC4 ELI with the interstitial limits written out |
| Hot chloride or crevice service | The Fe ceiling and oxygen content differ across "equivalent" grades | Ask for measured chemistry and coupon data in your medium |
| A GB material standard issued before 2007 | Its TA1 / TA2 may follow the older chemistry, not today’s TA1G / TA2G | State the chemistry edition on the PO, not just the standard number |
| A PO that says "or equivalent" | No enforceable chemistry, condition or certificate follows from it | Name standard + revision + UNS + condition + certificate type |
Outside this table, cross-referencing is a normal procurement step. Inside it, the grade name is not the controlling document. For mixed-material lines the same discipline applies across families — see how the alloy family matrix separates duties by stream, and note that nuclear-grade low-hafnium zirconium belongs to a qualified chain rather than general stock: the Zr702 / Zr705 grade note explains that split.
Ten lines turn an ambiguous grade name into a quotable specification. Send them together and the answer comes back on one basis.
| # | Field | Example entry |
|---|---|---|
| 1 | Grade, UNS and standard with revision | ASTM B265-20 Gr2 UNS R50400 — not "Gr2 equivalent" |
| 2 | Product form and its standard | Plate B265 / heat-exchanger tube B338 / seamless pipe B861 |
| 3 | Chemistry edition when citing GB | GB/T 3620.1-2016 TA2G versus the older TA2 |
| 4 | Condition | Annealed, cold-worked, 2H or STA — state it |
| 5 | ELI or standard | Gr23 per B348 (R56407) or F136 (R56401) |
| 6 | Aerospace specification | AMS 4928 with revision, if the drawing calls it |
| 7 | Certificate type and witness | EN 10204 3.1, or 3.2 with the witness named before manufacture |
| 8 | Full measured chemistry | Include O, N, H and C; light elements by E1409 / E1447 / E1941 |
| 9 | Heat traceability | Heat number hard-stamped on each piece and repeated on the MTC |
| 10 | Inspection scope | PMI plus laboratory light elements, UT class and NDE if required |
One extra line pays for itself: ask the supplier to confirm the standard revision in force at the time of manufacture, not the one on their website template. Standards are reissued, and a grade name with an old revision is a common source of a failed incoming inspection.
We are a stockholder plus light fabricator in Baoji, the centre of China’s Titanium Valley. This article is exactly the conversation we have with customers every week, so our working method is built around it:
Start with Titanium Plate, flange, fittings, bar or welding wire; each page gives the forms, sizes and certificate options.
|
Get a firm titanium quote within 24 hours Same-day dispatch from ~800 t of Baoji stock · cut-to-size and waterjet blanks · free drawing review by our engineering team · EN 10204 3.1 MTC with every lot. |
Request my quote →
No obligation. A named engineer replies, not an auto-responder. |
|
EN 10204 3.1 MTC on every lot · ISO 9001 quality system · ASTM / ASME / GB standard literacy · Third-party inspection (SGS / BV) on request · Mill heat & lot traceability · Export packing & full documentation |
Only under the 2007 version of GB/T 3620.1, where the grades matching ASTM Gr1-Gr4 were renamed TA1G-TA4G. In the current GB/T 3620.1-2016 the TA1-TA4 labels were restored with the older 1994 chemistry, so TA1 is closer to Grade 2 and TA2 closer to Grade 3. Always state the chemistry edition on the purchase order, not just the standard number.
It depends on the standard. ASTM B265, B348, B381 and B863 designate Grade 23 as UNS R56407. ASTM F136, the surgical-implant specification for Ti-6Al-4V ELI, uses UNS R56401. Many cross-reference charts print only R56401, which is the medical number applied to an industrial grade. Name the product standard first and let the UNS follow it.
Their nominal Ti-6Al-4V chemistry is close, but they are not identical: TC4 carries a 0.30% maximum iron limit, while ASTM Grade 5 allows 0.40%. The aluminium upper limit also differs between published sources, so verify the revision. For an aerospace drawing naming AMS 4928, or for a load-bearing implant needing ASTM F136 ELI, a generic TC4-for-Grade-5 substitution is not acceptable.
It is the most widely used European material number for Ti-6Al-4V. European sources disagree on whether 3.7164 or 3.7165 denotes aerospace Grade 5, industrial Grade 5 or the ELI Grade 23 variant, and no single unambiguous Werkstoff number is assigned to ELI. Treat the material number as a starting point and confirm the ASTM or AMS grade, condition and certificate instead.
No. Grade 23 is the extra-low-interstitial variant specified for toughness, cryogenic service and implants, not a higher-strength version. Its published minimum tensile is lower than Grade 5 - around 828 MPa versus 895 MPa for annealed product, with the exact figure depending on the standard revision and product form. Calling ELI 'a stronger Grade 5' is a factual error.
They answer different questions. The ASTM product standard defines chemistry, mechanical properties and test requirements; EN 10204 defines who signs the certificate and whether a third party witnessed it. An ASTM B348 mill test certificate is commonly issued as EN 10204 3.1. A 3.2 adds independent or purchaser witness and must be agreed before manufacture - it cannot be created by upgrading a 3.1 afterwards.
Write the product standard with its revision, the grade and UNS number, the condition, the certificate type and the inspection scope - for example ASTM B265-20 Grade 2 UNS R50400, annealed, EN 10204 3.1 with a hard-stamped heat number and measured oxygen, nitrogen, hydrogen and carbon. If you are citing a Chinese grade, add the chemistry edition, because TA2 under GB/T 3620.1-2016 is not the same as TA2G under the 2007 version.
Equivalence names a nominal chemistry match — it does not release a part. Under GB/T 3620.1–2016 the ASTM-matching pure grades are TA1G–TA4G, Grade 23 is R56407 in the ASTM B series but R56401 in F136, ELI has no single Werkstoff number, and TC4's 0.30% iron ceiling is not Grade 5's 0.40%. Write the standard with revision, UNS, condition, chemistry edition and certificate type on the PO, and the phrase “or equivalent” becomes unnecessary. Send your designation through our request a quotation page; a named engineer will reconcile it to ASTM / GB / EN and confirm stock and pricing within 24 hours.
Need a quote on this specification?
Click below and your email app opens with the 6-point RFQ already typed out. Just fill in your grade, size and quantity - no form, no captcha.
Prefer the web form? Open the inquiry page and paste the 6 points into the message box.
Baoji Titanium Valley · ~800 t stock · cut-to-size · drawing-based machining · ASTM / ASME / GB · export-ready · same-day quote.
Contact Person: Wang Xiaoning
Tel: +86-917-355-7966
Email: [email protected]
WhatsApp: +86 188 2967 9311
Company: Shaanxi Qianyi Tuoda Technology Co., Ltd
Address: Floor 4, Building 4, No. 188 Gaoxin Avenue, High-tech Zone, Baoji City, Shaanxi Province, China