Commercially pure titanium (Grades 1–4) cannot be hardened by heat treatment. It is single-phase alpha at room temperature: you can anneal it to restore ductility or stress-relieve it after forming and welding, but the strength in the box was set at the melt by oxygen and iron, and, if you ordered it cold-worked, by the amount of reduction. Ti-6Al-4V (Grade 5) is a different metal: mill annealed, solution treated and aged (STA), beta annealed and stress-relieved conditions move tensile strength from about 895 MPa in the annealed state to over 1,100 MPa after STA — while fracture toughness moves in the opposite direction. In CP titanium, oxygen is the real strength lever: roughly 50 MPa of tensile strength per 0.1 wt% oxygen, which is why the certificate, not the furnace, decides the grade. Boundary: published annealing windows disagree between mills and data sheets, sometimes by more than 100°C. This article gives the ranges and the verification action, not one universal cycle. Ask your supplier for the actual cycle and coupon data in your own section and condition. See our ASTM / GB / EN equivalence guide for the chemistry limits behind these grades.
How to read the numbers. We are a stockholder and light fabricator in Baoji, not a heat-treatment standards body. Every temperature below is an indicative published range, attributed to the data sheet or technical note it came from. Where sources conflict, the conflict is shown in a table and the answer is a verification step, never a invented single value. The alpha-case threshold and the oxygen-strength relationship are quoted from producer and technical literature with the source named. None of this is a heat-treatment procedure for your part: final cycles must come from the governing material specification, your drawing, or an approved process route. If a number matters to a safety-critical order, ask your supplier for coupon data from a run in the same section and condition.
| Topic | Indicative value | Mechanism | What to freeze on the RFQ |
|---|---|---|---|
| CP Gr1–4 | Not hardenable by heat treatment | Single-phase alpha; strength from O, Fe and cold work | Name O limit and condition, not a hardness target |
| CP soft anneal | ~600–760°C (sources differ) | Restores ductility after cold work | State the standard default; ask for the actual cycle |
| CP stress relief | ~450–600°C | Reduces forming / welding residual stress | Say whether it is required after welding |
| Oxygen in CP | ~50 MPa tensile per 0.1 wt% O | Solid-solution strengthening | Require measured O on the MTC |
| Gr5 mill anneal | ~700–790°C, air cool | Balanced strength and ductility; default condition | “Mill annealed to B348” plus minimums |
| Gr5 STA | ~913–954°C + age ~524–552°C | Highest strength, lower ductility and toughness | Quench, section size and aging window |
| Gr5 beta anneal | ~1,000–1,065°C | Fracture toughness and creep, lower fatigue | Only when the drawing calls for it |
| Alpha case | Risk above ~427°C in air | Hard, brittle oxygen-rich surface layer | Vacuum / argon; specify removal and acceptance |
| Cold-worked temper | Named by reduction or temper | Raises strength, lowers formability | Ask for the numeric tensile, not the temper name |
How to use this table: each row is a question the condition line on your quotation should answer. A supplier who can explain all nine without checking is usually the one holding the stock that actually matches the drawing. For the price effect of choosing one condition over another, see our why two titanium quotes differ.
The word “heat treatment” covers two unrelated situations. For commercially pure titanium (Grades 1 to 4), heat treatment can soften or relieve but cannot strengthen: the metal is alpha-phase all the way to the beta transus, so there is no martensitic transformation to exploit. For Ti-6Al-4V (Grade 5), heat treatment is a genuine strength lever because the alloy is alpha-beta and can be solution treated, quenched and aged.
That distinction decides most RFQs. If a supplier offers to “heat treat Grade 2 to higher strength”, they are describing something other than certified CP titanium. If a buyer orders Grade 5 “annealed” for a fatigue-critical shaft without stating which anneal, they have left the largest property variable undefined. The rest of this article is about making that line explicit. Start with our Titanium Plate overview or Grade 5 bar stock if you need the product background first.
Steel hardens because iron changes crystal structure with temperature and carbon traps that change on cooling. Titanium has no equivalent route in the CP grades. Above the beta transus the body-centred cubic beta phase exists, but cooling a CP grade back down does not create a hard metastable structure you can temper to a target strength in the way a steel shop would.
Producers state this plainly: Grades 1, 2, 3 and 4 cannot be strengthened by heat treatment. What they can do is soft anneal to recover ductility after rolling or forming, and stress relieve to reduce residual stress after machining or welding. Anything sold as a strengthened CP condition is cold worked, and the strength is a function of reduction, not of the furnace. This is the single most useful correction to carry into a supplier conversation.
Because heat treatment cannot raise CP strength, mills control it at the melt. Oxygen, iron, nitrogen and carbon sit in the alpha lattice and impede dislocation motion. Oxygen is the strongest of them: technical literature puts the effect at roughly 50 MPa of tensile strength per 0.1 wt% oxygen. ASTM B265 sets Grade 2 oxygen at 0.25 wt% maximum, and each grade up the CP family buys strength by allowing more interstitial content.
| Grade | Interstitial ceiling | Strength / formability | Typical use |
|---|---|---|---|
| Grade 1 | Lowest interstitial ceiling | Most formable, lowest strength | Deep drawing, complex forming |
| Grade 2 | O ≤0.25 wt% (B265) | Workhorse balance | Plate, tube, vessels, marine |
| Grade 3 | Higher O and Fe ceiling | Higher strength, less forming margin | Structural parts where forming is limited |
| Grade 4 | Highest O and Fe ceiling | Highest CP strength, least ductility | Strength-driven CP parts |
The practical consequence: a certificate showing the measured oxygen value tells you more about the strength of a CP plate than a statement about its furnace cycle. That is why our EN 10204 3.1 mill certificate page lists measured interstitials as a field to request, and why the grade equivalence guide compares oxygen ceilings across ASTM, GB and EN — two grades that look equivalent on a chart can sit at different points on this strength scale.
These are different operations with different purposes and different temperatures. Annealing takes the metal to a condition of minimum strength and maximum ductility, usually followed by air cooling. Stress relieving uses a lower sub-anneal temperature to reduce residual stress from welding, forming or heavy machining while largely preserving the strength already in the part.
| Condition | Definition | When it is used | Grades |
|---|---|---|---|
| Annealed | Heat treated to soften and restore ductility | Default for most mill product | Gr1–4, Gr5 |
| Stress relieved | Sub-anneal cycle to reduce residual stress | After forming, machining or welding | Gr1–4, Gr5 |
| Cold-worked / temper | Strength raised by reduction, not heat | Thin strip, wire, tube | Gr1–4 mainly |
| Mill annealed | Producer standard anneal, no extra cycle | Default Gr5 condition | Gr5, B348 / AMS 4928 |
| STA | Solution treat + quench + age | Maximum strength route | Gr5, AMS 4967 family |
| Beta annealed | Above beta transus, lamellar structure | Toughness / creep over fatigue | Gr5, drawing-driven |
Confusing the two causes real orders to fail. A deep-drawn part annealed to restore formability must not be shipped stress-relieved only; a welded assembly stress-relieved at a lower temperature keeps strength that a full anneal would remove. Write the word that matches the purpose on the PO, and let the mill choose the cycle within the governing standard.
The fastest way to remove this ambiguity is to send the same condition fields to every supplier. These are the lines we ask for; copy them into your enquiry and the answers come back on one basis.
|
What to send us for an exact titanium quote Copy these nine lines into your enquiry. A complete spec means a firm price on the first reply, not a second email asking for the grade. |
||||||||||||||||||||
|
||||||||||||||||||||
|
Ready? Copy the nine lines above into the Requirement Details box on our Request a Quotation page and we will come back with a firm price and a dispatch date within 24 hours. |
A search for the annealing temperature of Grade 2 returns several different answers. They are not all wrong; they are producer practices for different products, section sizes and furnaces. The spread is large enough that a PO naming a single temperature can be impossible to satisfy exactly.
| Source | Grade 2 anneal | Grade 5 mill anneal | Nature of source |
|---|---|---|---|
| Rolled Alloys datasheet | 649–788°C, 15 min–2 h, air | 704–788°C, 2 h, air | Commercial producer data sheet |
| HWN Titan datasheet | 600–700°C soft anneal | Not stated | European producer data sheet |
| materialref.com | 650–760°C, 1–2 h, air | Not stated | Reference database |
| Technical guide (ATI / Carpenter cycles) | Not stated | 691–790°C mill anneal | Compiled producer cycles |
| Read-out | Window spans >100°C across sources | Window spans ~100°C | Specify the standard, not a lone temperature |
The correct RFQ wording is “annealed to ASTM B265, revision X”, not a temperature chosen from one data sheet. If your drawing genuinely needs a specific cycle, add it as an explicit requirement and agree the inspection that proves it. Where sources conflict we do not pick a winner: ask the mill for the cycle it will run and for coupon data from the same section and condition. This is the same discipline we apply to the tolerance and certificate fields in our China sourcing guide.
Titanium’s affinity for oxygen is an advantage in service and a problem in the furnace. Above roughly 427°C, exposed titanium absorbs oxygen into the surface, producing a hard, brittle alpha-stabilised layer called alpha case. It is not visible to the naked eye in its early stages, and it is a fatigue crack initiation site.
| Observation | What happens | Required control |
|---|---|---|
| Above ~427°C in air | Oxygen diffuses into the surface | Vacuum or high-purity argon furnace |
| Hard, brittle alpha layer | Cracks can start there under fatigue | Pickling or centreless grinding after the cycle |
| Welding is the same risk | Molten and hot metal react with O, N, H | Shield weld pool, HAZ and back side until cool |
| Colour is the field signal | Silver / light straw acceptable; blue / grey rejected | Write the acceptance tint into the procedure |
The control is straightforward but non-negotiable: any thermal cycle above that range runs in vacuum or high-purity argon, and the surface layer is removed chemically or mechanically afterwards. Welding is the same reaction at a smaller scale, which is why the failure casebook treats back purging and weld colour as acceptance criteria rather than cosmetic detail. If your part will be fatigue-loaded, write the alpha-case removal and acceptance method into the PO.
Ti-6Al-4V is where heat treatment pays. The same chemistry can be delivered in several conditions whose tensile strength, ductility, toughness and fatigue behaviour differ enough that substituting one for another is a design change, not a logistics choice.
| Route | Indicative cycle | Property outcome | Where it belongs |
|---|---|---|---|
| Mill anneal | ~700–790°C, 1–4 h, air cool | ~895 MPa min tensile | Balanced; ~80% of uses |
| STA | Solution ~913–954°C, water quench; age ~524–552°C | ~1,100–1,200 MPa tensile | Peak strength, lower ductility |
| Beta anneal | Above beta transus, ~1,000–1,065°C | Lower tensile, higher toughness | Damage tolerance and creep |
| Duplex anneal | High anneal + lower stabilising step | Balanced strength / ductility | Marine and SCC-sensitive service |
| Stress relief / PWHT | ~480–650°C, 1–4 h | Little change to tensile | Welded and machined parts |
Mill annealed is the default and suits roughly four out of five applications. STA is a high-strength route for fasteners and structures where the drawing demands it, with a real penalty in ductility and fracture toughness. Beta annealing buys toughness and creep resistance at the cost of fatigue strength and machinability, so it belongs in damage-tolerant aerospace designs rather than general bar stock. A Grade 5 bar order should therefore state the condition as explicitly as the diameter.
STA reaches peak properties only if the section quenches fast enough to suppress diffusion-controlled alpha precipitation. Thin sheet and small bar can hit the upper end of the strength range; thick sections cool too slowly at the core and fall short. Producer notes put the practical limit at around one inch for full through-hardening in some products, which is why large forgings are rarely certified to the highest STA minimums.
The buyer’s action is to tie the strength requirement to the section, not to the grade name. Ask for the mechanical minimums at your actual thickness and the quench medium the supplier will use. If a quote promises aerospace STA strength on a heavy section without that conversation, the number will not survive testing. Our stock-size dispatch is deliberately from annealed stock, because that is the condition in which most sections are actually usable.
A higher-strength condition is not an upgrade in every service. Raising oxygen or cold work in CP titanium reduces ductility and formability; STA in Grade 5 reduces elongation and fracture toughness; beta annealing improves toughness but lowers fatigue strength. Galling, stress-corrosion behaviour and weldability can also move with the condition.
Choose the condition the part needs, then stop. A welded vessel that will be formed and requalified wants annealed CP material, not the highest strength plate on the shelf. A shaft in a tight section may genuinely need STA Grade 5. If you are unsure which grade the medium calls for before you choose a condition, the tube selection guide and the failure casebook are the right starting point.
Thin titanium strip, wire and some tube are sold in cold-worked conditions named by reduction or by a temper designation such as quarter-hard, half-hard or full-hard. The temper raises strength and lowers formability without any strengthening heat treatment. The trap is that temper names and the corresponding minimum tensile values are not interchangeable across suppliers or product forms.
Ask for the numeric minimum tensile and yield on the certificate, together with the reduction or temper designation, rather than relying on the label alone. The same advice applies to welding wire and to thin strip used for formed parts: a two-step forming operation that worked with one supplier’s half-hard coil may crack with another’s. Our cut-to-size service starts from declared stock conditions so the temper is known before cutting.
Post-weld heat treatment has a narrow, useful job: it lowers residual stress and distortion in a welded or heavily machined part, and it is normally sequenced before final machining. It does not change the chemistry of the weld zone.
| Problem | Does PWHT fix it? | Correct action |
|---|---|---|
| Residual stress from welding or heavy machining | Reduced | Yes, within an agreed cycle |
| Distortion risk before final machining | Lowered | Yes, sequence it before finish cuts |
| Oxygen / nitrogen contaminated weld metal | Not repaired by heating | No — remove and re-weld under purge |
| Hydrogen pickup | Not a heat-treatment fix | No — control at source, verify chemistry |
| Wrong grade or mixed heat | Unchanged by the cycle | No — PMI and heat-number traceability |
The distinction matters because a contaminated weld is the most common expensive failure in reactive-metal fabrication. Heat cannot undo oxygen or nitrogen pickup; only removal and a re-weld under proper purge can. If your fabrication route includes a PWHT step, agree the cycle and the sequence with the fabricator before the first weld, not after a failed inspection.
Section 5 showed that published windows differ by more than 100°C. The reason is practical: mills optimise for their product mix, furnace type and section range, and the standard specifies an outcome rather than one universal recipe. A clause that names a single temperature without a furnace, hold time and cooling method can therefore be commercially unworkable.
The verification sequence is simple. First, name the governing standard and revision. Second, ask the supplier which cycle it will run. Third, ask what inspection proves the resulting condition — tensile, hardness, or both. Fourth, require coupon data from the same section if the part is critical. This turns a disputed number into an auditable answer, and it is the approach we take with every specification question in our standards guide.
If your drawing says only “annealed” or “Gr5”, send it through our request a quotation page. A named engineer will return the reconciled condition, the mechanical minimums and the certificate wording in writing — within 24 hours — so the three suppliers on your list are quoting the same material.
There are orders where focusing on the furnace distracts from the variable that actually decides success. Naming them is part of a straight technical answer.
| Condition | Why condition is not the main lever | What to do instead |
|---|---|---|
| Corrosion-critical service | Condition does not replace grade selection for the medium | Choose by medium; request coupon data — see the failure casebook |
| An aerospace or implant order | AMS or F136 revision controls the route, not a generic anneal | Quote to the named specification and revision |
| Aerospace Gr5 STA in thick section | Hardenability is limited; the core may miss full properties | Confirm section size and quench route |
| A low-cost CP order | Paying for a special thermal cycle adds no strength | Buy to the standard annealed condition |
| US defence work | Chinese melt is not qualified under DFARS specialty-metal rules | Decline honestly; point buyer to a qualified chain |
Outside this table, condition is a normal and important specification field. Inside it, the governing document or the service medium controls and the thermal route follows. The same logic applies across our alloy family, where a heat-treatment answer is often the wrong answer to a corrosion question.
Twelve lines make a condition unambiguous enough to quote and to inspect. Send them together so the answers come back on one basis.
| # | Field | Example entry |
|---|---|---|
| 1 | Grade + UNS + revision | Gr2 UNS R50400 / Gr5 UNS R56400 |
| 2 | Product standard | Plate ASTM B265 / bar B348 / tube B338 |
| 3 | Condition | Annealed / stress relieved / cold-worked / STA |
| 4 | Cycle definition | “Per the standard” unless drawing specifies temperature |
| 5 | Furnace atmosphere | Vacuum or high-purity argon above ~427°C |
| 6 | Alpha-case control | Removal method and acceptance tint / depth |
| 7 | Mechanical minimums | Room-temperature tensile, yield, elongation |
| 8 | Hardness, if required | Range + method, agreed before manufacture |
| 9 | Measured interstitials | O / N / H / C values on the certificate |
| 10 | PWHT | Required? cycle, and before or after machining |
| 11 | Certificate type | EN 10204 3.1; 3.2 with named witness if needed |
| 12 | Heat-number traceability | Hard stamp or permanent mark across the lot |
The two lines most often left out are the furnace atmosphere and the alpha-case acceptance method. Both matter more than the nominal temperature, because they determine whether the surface you receive is the surface you specified. For the complete commercial picture behind these fields, pair this checklist with the quote-comparison guide.
We are a stockholder plus light fabricator in Baoji, the centre of China’s Titanium Valley. Condition is a stock question for us, not a furnace we have to sell you:
Start with plate, tube, bar, wire, flange or fittings; each page lists the forms, sizes and condition options that matter for that product.
|
Get a firm titanium quote within 24 hours Same-day dispatch from ~800 t of Baoji stock · cut-to-size and waterjet blanks · free drawing review by our engineering team · EN 10204 3.1 MTC with every lot. |
Request my quote →
No obligation. A named engineer replies, not an auto-responder. |
|
EN 10204 3.1 MTC on every lot · ISO 9001 quality system · ASTM / ASME / GB standard literacy · Third-party inspection (SGS / BV) on request · Mill heat & lot traceability · Export packing & full documentation |
No. Commercially pure titanium grades 1 to 4 are single-phase alpha at room temperature and do not harden by quenching or aging the way steel or Ti-6Al-4V does. Their strength comes from controlled interstitial content, mainly oxygen and iron, and from cold work. You can anneal to soften, or stress relieve after forming or welding, but if you need more strength you choose a higher-oxygen CP grade or a cold-worked temper, not a furnace cycle.
It means the material received a thermal cycle that leaves it in a soft, ductile, stable condition, normally the default condition for ASTM B265 plate or B348 bar. It does not define one temperature: published anneal windows for Grade 2 span roughly 600 to 760 degrees Celsius depending on the source. Specify annealing to the named product standard and revision, and ask the mill for the actual cycle, rather than inventing a temperature that no two data sheets agree on.
Oxygen is the strongest solid-solution strengthener in commercially pure titanium. Technical literature puts the change at roughly 50 MPa of tensile strength for each 0.1 weight percent of oxygen, which is why ASTM limits oxygen tightly and why the certificate must show the measured value. More oxygen buys strength and costs ductility and formability, so it is a grade-selection decision, not something to add after manufacture.
Mill annealed is the producer default: roughly 700 to 790 degrees Celsius with an air cool, giving equilibrium alpha plus beta, useful ductility and about 895 MPa minimum tensile. STA means solution treatment around 913 to 954 degrees Celsius, a water quench and aging around 524 to 552 degrees Celsius, reaching roughly 1,100 to 1,200 MPa tensile with lower elongation and toughness. STA is specified for high-strength parts; it is not an automatic upgrade for general stock.
Alpha case is a hard, brittle, oxygen-enriched surface layer formed when titanium is heated in air above roughly 427 degrees Celsius. It can initiate fatigue cracks and must be removed by pickling or grinding after any hot process. The same reaction is why welding needs argon shielding of the pool, the heat-affected zone and the back side until the metal cools below that range.
No. A stress-relief cycle reduces residual stress but cannot restore a weld zone that picked up oxygen, nitrogen or hydrogen, because the damaged chemistry is already in the metal. A blue, grey or powdery white weld indicates contamination: cut it out and re-weld with correct purging. Read our failure casebook for the colour scale and the backing-gas rule.
Write the grade with UNS and revision, the product standard, and the condition in one line, for example Grade 5 bar to ASTM B348, mill annealed. Add mechanical minimums, measured oxygen and iron on the certificate, the certificate type, and whether post-weld heat treatment is required. If the part is heat treated after receipt, name the atmosphere and how alpha case will be removed and accepted.
CP titanium is not hardenable by heat; Ti-6Al-4V is, and the chosen route changes the part. Oxygen and cold work set the strength of Grades 1 to 4, roughly 50 MPa per 0.1 wt% oxygen. Mill annealed, STA, beta annealed and stress-relieved Grade 5 sit at very different points on the strength-toughness scale. Where published windows disagree, specify the governing standard and ask for the actual cycle and coupon data. Above roughly 427°C, control the atmosphere and remove any alpha case. Send the twelve-line checklist through our request a quotation page; a named engineer will return the reconciled condition and certificate wording within 24 hours.
Need a quote on this specification?
Click below and your email app opens with the 6-point RFQ already typed out. Just fill in your grade, size and quantity - no form, no captcha.
Prefer the web form? Open the inquiry page and paste the 6 points into the message box.
Baoji Titanium Valley · ~800 t stock · cut-to-size · drawing-based machining · ASTM / ASME / GB · export-ready · same-day quote.
Contact Person: Wang Xiaoning
Tel: +86-917-355-7966
Email: [email protected]
WhatsApp: +86 188 2967 9311
Company: Shaanxi Qianyi Tuoda Technology Co., Ltd
Address: Floor 4, Building 4, No. 188 Gaoxin Avenue, High-tech Zone, Baoji City, Shaanxi Province, China